I- CVD growth update: The following picture shows the CVD growth for WS2. The yield is not very High like MoS2, it is only on the center sample and triangle size up to 80um. To improve the growth, we need to reduce the sulfur flux, and increase the Tungsten trioxide (WO3) flux by changing temperature or quantities. Also, we should increase the growth time. II- Device fabrication: Dos test for SU8: Spin 2000 rpm , the recipe is under my name Abdul. Bake 105 (actual ~95) for 60s. Dose 3.3 c/um, Current 100pa, bake for 60s at 105c. Developing for 90s. Place the sample on the hot plate and increase the temp. To 190c (~170c) for 45min. Lift off problem using gold at CUNY: I tried lower power 40% for the gold in order to deposit